Bobon Copper

Guides

Phosphor bronze or beryllium copper for springs (C5210 vs C17200)

C5210 (CuSn8, 470 to 885 MPa, about 12 % IACS) is the economical spring alloy for most contacts and needs no heat treatment after forming. C17200 reaches above 1,300 MPa after age hardening, conducts 22 to 28 % IACS and keeps its spring force better at elevated temperature and over many cycles; choose it for small, highly stressed springs, high-cycle contacts and parts that run warm.

Side-by-side data

C5210C17200
UNSC52100C17200
EquivalentsEN CuSn8 / CW453K; JIS C5210; GB QSn8-0.3EN CuBe2 / CW101C; JIS C1720; GB QBe2 (TBe2)
Composition %Sn 7.0 – 9.0, P 0.03 – 0.35, Cu + Sn + P ≥ 99.7Be 1.80 – 2.00, Co + Ni ≥ 0.20, Co + Ni + Fe ≤ 0.60
Conductivity %IACS≈ 1222 – 28
Tensile strength MPa470 – 885410 – 1520
Tempers1/2H, H, EH, SH, ESHA (TB00), 1/4H (TD01), 1/2H (TD02), H (TD04), AT (TF00), 1/2HT (TH02), HT (TH04)
Elastic modulus110 GPa131 GPa
Density8.80 g/cm³8.25 g/cm³

Tensile strength is the range across supplied tempers. Full composition, tempers and physical properties are on each grade page.

Choose C5210 when

Choose C17200 when

Notes

C17200 is supplied either age-hardenable (formed, then heat treated) or mill-hardened (ready to use); the grade page explains the choice. It contains beryllium, so grinding, welding or machining dust should be handled under the supplier's safety guidance. Copper-titanium is another high-strength option; see the beryllium copper vs copper-titanium guide.

Questions buyers ask

Can C17200 be bought already hardened?

Yes. Mill-hardened tempers are supplied ready to stamp, with no heat treatment at your plant. They are less formable than the age-hardenable tempers, so tight bends may need the age-hardenable route.

Need a recommendation for a specific part?

Tell us the part function, strip thickness and performance targets. We reply within one working day, and sample coils are available for comparative trials.