Nickel silver vs phosphor bronze (C7521 vs C5210)
C7521 nickel silver (CuNi18Zn20, 448 to 586 MPa, about 6 % IACS) is chosen for its silver-white colour, tarnish resistance and good solderability, which suit shielding cans, crystal and component housings and visible parts. C5210 phosphor bronze is stronger (up to 885 MPa) and conducts about twice as well, so it is the better choice for spring contacts.
Side-by-side data
| C7521 | C5210 | |
|---|---|---|
| UNS | C75200 | C52100 |
| Equivalents | EN CuNi18Zn20 / CW409J; JIS C7521; GB BZn18-18 | EN CuSn8 / CW453K; JIS C5210; GB QSn8-0.3 |
| Composition % | Cu 63.0 – 66.5, Ni 16.5 – 19.5, Mn ≤ 0.50, Fe ≤ 0.25 | Sn 7.0 – 9.0, P 0.03 – 0.35, Cu + Sn + P ≥ 99.7 |
| Conductivity %IACS | 6 | ≈ 12 |
| Tensile strength MPa | 448 – 586 | 470 – 885 |
| Tempers | H01, H02, H04 | 1/2H, H, EH, SH, ESH |
| Elastic modulus | 124 GPa | 110 GPa |
| Density | 8.75 g/cm³ | 8.80 g/cm³ |
Tensile strength is the range across supplied tempers. Full composition, tempers and physical properties are on each grade page.
Choose C7521 when
- The part is a shielding can or housing that is soldered to the board
- Appearance and tarnish resistance matter
- Low conductivity is acceptable
Choose C5210 when
- The part is a spring contact that carries current
- Higher strength or fatigue resistance is needed
- The part is plated anyway, so colour does not matter
Notes
Nickel silver contains no silver; the name comes from its colour. For shielding where higher conductivity is wanted, tin-plated C2680 brass or C19400 are also used.
Questions buyers ask
Is nickel silver the same as white copper?
In Chinese usage 白铜 covers both copper-nickel (such as B10) and copper-nickel-zinc. C7521 is the copper-nickel-zinc type, also called 锌白铜 or 洋白铜 (GB BZn18-18).
Need a recommendation for a specific part?