Terminals that run hot: matching the alloy's conductivity to the current
Many current-carrying terminals are made from materials chosen for their spring properties or their cost: brass and phosphor bronze at 13 to 28 % IACS, pure nickel at about 25 %, or copper-nickel-tin spring alloys at 40 to 50 %. These serve well at signal currents. As current rises, the strip itself heats, and a more conductive alloy becomes the simplest fix: C19010 at 55 % or more, C19720 and C18140 at 80 % or more, and C15100 at 90 % or more. Halving the resistance roughly halves the heat generated in the same cross-section.
Candidate grades
| NB109 | NB105 | C19010 | C19720 | C18140 | C151 | |
|---|---|---|---|---|---|---|
| UNS | C19025 | C19020 | C19010 | C19720 | C18140 | C15100 |
| Equivalents | JASO JC400 | JASO JC400 | EN CuNiSi (low-alloyed) | – | EN CuCrZr (low-alloyed) | JIS C1510 |
| Composition % | Ni 1.0, Sn 0.90, P 0.05 | Ni 1.0, Sn 0.50, P 0.05 | Ni 0.8 – 1.8, Si 0.15 – 0.35, P 0.01 – 0.05 | Fe 0.05 – 0.50, Mg 0.06 – 0.20, P 0.05 – 0.15, Sn ≤ 0.20, Zn ≤ 0.20, Ni ≤ 0.10, Pb ≤ 0.05, Mn ≤ 0.05 | Cr 0.15 – 0.45, Zr 0.05 – 0.25, Si 0.005 – 0.05 | Zr 0.05 – 0.15, Cu ≥ 99.80 |
| Conductivity %IACS | 40 | 50 | ≥ 55 | 80 | 85 | ≥ 90 |
| Tensile strength MPa | 440 – 590 | 300 – 550 | 360 – 590 | 365 – 505 | 393 – 490 | 245 – 490 |
| Tempers | 1/2H, H, EH | 1/4H, 1/2H, H, EH | 1/4H, 1/2H, H, EH, SH | 1/2H, H, EH | H04, H08 | 1/4H, 1/2H, 3/4H, H, EH, SH |
| Elastic modulus | 130 GPa | 130 GPa | 127 GPa | 118 GPa | 117 GPa | 118 GPa |
| Density | 8.9 g/cm³ | 8.9 g/cm³ | 8.9 g/cm³ | 8.84 g/cm³ | 8.91 g/cm³ | 8.94 g/cm³ |
Tensile strength is the range across supplied tempers. Full composition, tempers and physical properties are on each grade page.
Why a terminal overheats
- Bulk resistance: heat in the strip rises in proportion to its resistivity. A 40 % IACS alloy has twice the resistivity of an 80 % alloy, and pure nickel or phosphor bronze has three to six times.
- Contact resistance: as the spring relaxes with heat and time, contact force falls and resistance at the interface rises. This is why stress relaxation resistance matters as much as conductivity.
- The two feed each other: a hotter terminal relaxes faster, which raises resistance and temperature again.
Choosing the material
- Signal terminals and small female terminals where spring force leads: NB109 and NB105 remain the right choice, with proven stress relaxation resistance.
- The same design carrying more current: C19010, which stays close in strength while conducting at 55 % IACS or more.
- Power terminals that run warm: C19720 or C18140. Both conduct at 80 % IACS or more and resist softening and stress relaxation; the spring section usually needs checking because strength is lower.
- Blades, tabs and busbars that do not act as springs: C15100, or pure copper where strength is not needed.
- Parts now made in pure nickel for weldability: nickel-plated copper alloy keeps a nickel surface while the copper core carries the current.
- Split the functions: a high-conductivity blade with a separate spring clip in a stronger alloy often outperforms a single compromise material.
What to test
- Temperature rise at rated and peak current, on formed and plated parts
- Contact force and contact resistance after heat ageing
- Forming and bend behaviour in the existing die
Notes
Tell us what the terminal is made from today, the current, the allowed temperature rise, the strip thickness and the plating. We supply sample coils of two or three candidate grades in the same thickness, so that a comparative temperature-rise and heat-ageing test can be run on real terminals.
Questions buyers ask
Can a higher-conductivity alloy run in the existing die?
Sometimes. C19010 is close enough in strength to copper-nickel-tin spring alloys that many dies run with minor adjustment. C19720, C18140 and C15100 are softer, so springback and contact force change and the spring geometry should be reviewed.
Is higher elongation the answer to overheating?
No. Elongation affects forming, not heating. Heating is governed by conductivity and by how well the alloy keeps its contact force at temperature.
Need a recommendation for a specific part?
Tell us the part function, strip thickness and performance targets. We reply within one working day, and sample coils are available for comparative trials.
Material development support