Terminals that run hot: matching the alloy's conductivity to the current

Many current-carrying terminals are made from materials chosen for their spring properties or their cost: brass and phosphor bronze at 13 to 28 % IACS, pure nickel at about 25 %, or copper-nickel-tin spring alloys at 40 to 50 %. These serve well at signal currents. As current rises, the strip itself heats, and a more conductive alloy becomes the simplest fix: C19010 at 55 % or more, C19720 and C18140 at 80 % or more, and C15100 at 90 % or more. Halving the resistance roughly halves the heat generated in the same cross-section.

Candidate grades

NB109NB105C19010C19720C18140C151
UNSC19025C19020C19010C19720C18140C15100
EquivalentsJASO JC400JASO JC400EN CuNiSi (low-alloyed)–EN CuCrZr (low-alloyed)JIS C1510
Composition %Ni 1.0, Sn 0.90, P 0.05Ni 1.0, Sn 0.50, P 0.05Ni 0.8 – 1.8, Si 0.15 – 0.35, P 0.01 – 0.05Fe 0.05 – 0.50, Mg 0.06 – 0.20, P 0.05 – 0.15, Sn ≤ 0.20, Zn ≤ 0.20, Ni ≤ 0.10, Pb ≤ 0.05, Mn ≤ 0.05Cr 0.15 – 0.45, Zr 0.05 – 0.25, Si 0.005 – 0.05Zr 0.05 – 0.15, Cu ≥ 99.80
Conductivity %IACS4050≥ 558085≥ 90
Tensile strength MPa440 – 590300 – 550360 – 590365 – 505393 – 490245 – 490
Tempers1/2H, H, EH1/4H, 1/2H, H, EH1/4H, 1/2H, H, EH, SH1/2H, H, EHH04, H081/4H, 1/2H, 3/4H, H, EH, SH
Elastic modulus130 GPa130 GPa127 GPa118 GPa117 GPa118 GPa
Density8.9 g/cm³8.9 g/cm³8.9 g/cm³8.84 g/cm³8.91 g/cm³8.94 g/cm³

Tensile strength is the range across supplied tempers. Full composition, tempers and physical properties are on each grade page.

Why a terminal overheats

Choosing the material

What to test

Notes

Tell us what the terminal is made from today, the current, the allowed temperature rise, the strip thickness and the plating. We supply sample coils of two or three candidate grades in the same thickness, so that a comparative temperature-rise and heat-ageing test can be run on real terminals.

Questions buyers ask

Can a higher-conductivity alloy run in the existing die?

Sometimes. C19010 is close enough in strength to copper-nickel-tin spring alloys that many dies run with minor adjustment. C19720, C18140 and C15100 are softer, so springback and contact force change and the spring geometry should be reviewed.

Is higher elongation the answer to overheating?

No. Elongation affects forming, not heating. Heating is governed by conductivity and by how well the alloy keeps its contact force at temperature.

Need a recommendation for a specific part?

Tell us the part function, strip thickness and performance targets. We reply within one working day, and sample coils are available for comparative trials.